Table 1 Shear bond strength (mean and standard deviation) of the tested materials on dentine after 2 d, 7 d and 14 d

From: Shear bond strength of Biodentine, ProRoot MTA, glass ionomer cement and composite resin on human dentine ex vivo

Material 2 d 7 d 14 d
ProRoot MTA 0.0a 0.85 (±1.42)a* 4.96 (±4.54)a**
Biodentine 3.14 (±1.09)b 9.75 (±2,19)b* 9.34 (±1.01)b*
ChemFil rock (GIC) 10.92 (±5.69)c 9.73 (±4.03)b 9.94 (±1.44)b
X-trabase (composite resin) + 32.74 (±4.66)d 32.75 (±4.61)c 30.48 (±4.43)c
Futurabond DC (dentine adhesive)
  1. Values with the same superscript letters were not statistically different at p = 0.05.
  2. * = statistically significant difference of the shear bond strength values in comparison to the values at the 2 d observation period (p < 0.05).
  3. ** = statistically significant difference of the shear bond strength values in comparison to the values at the 7 d observation period (p < 0.05).
  4. All values are given in MPa. The statistical evaluation was performed using ANOVA and Tukey-test (p < 0.05).